Grades 304 and 316 make up most of the stainless steel piping specified worldwide. They look identical on the rack, but one contains molybdenum and the other does not, and that single difference decides how long the pipe lasts in chloride service.
Composition compared
| Grade | UNS | Carbon, max % | Chromium % | Nickel % | Molybdenum % | Approx. PREN |
|---|---|---|---|---|---|---|
| 304 | S30400 | 0.08 | 18.0–20.0 | 8.0–10.5 | — | 19 |
| 304L | S30403 | 0.03 | 18.0–20.0 | 8.0–12.0 | — | 19 |
| 316 | S31600 | 0.08 | 16.0–18.0 | 10.0–14.0 | 2.0–3.0 | 24 |
| 316L | S31603 | 0.03 | 16.0–18.0 | 10.0–14.0 | 2.0–3.0 | 24 |
Ranges are typical of ASTM A240 and A312. Check the exact limits in the product standard on your purchase order.
Corrosion resistance
Both grades resist general corrosion in water, food products and many mild chemicals. The difference shows up with chlorides, from seawater, de-icing salts, cleaning chemicals or process streams. Molybdenum in 316 strengthens the passive film and raises resistance to pitting and crevice corrosion, which is why its PREN is around 24 compared with about 19 for 304.
Where chloride levels are high, or temperatures rise above about 50 °C in chloride service, even 316L can pit or suffer stress corrosion cracking. That is the point to look at duplex 2205 or super duplex.
Welding and the L grades
When standard 304 or 316 is held between about 425 and 815 °C, for example in the heat-affected zone of a weld, chromium carbides can form at the grain boundaries. The metal next to them loses chromium and can corrode along the grain boundaries, a problem called sensitisation.
The L grades cap carbon at 0.03%, leaving too little carbon to form harmful carbides during normal welding. Most pipe today is dual-certified 304/304L or 316/316L, meeting the low carbon limit of the L grade and the strength of the standard grade.
Which grade to choose
- 304/304L: potable water, food and dairy, architectural, general process piping without chlorides.
- 316/316L: coastal and marine atmospheres, pharmaceutical, chemical processing, brackish water and cleaning chemicals containing chlorides.
- 304H or 316H: service above about 500 °C where creep strength matters.
316L typically costs more than 304L because of its molybdenum and higher nickel content. In chloride service the extra cost is usually recovered many times over in service life.
Explore our stainless steel grades or stainless steel pipes and tubes.